娇妻借朋友高h繁交h,公交车伦流澡到高潮hnp,六月婷婷网视频在线观看,天堂√最新版中文在线

Language:CHINESESENGLISH

Home > News > Flame correct way construction steel welding deformation What?
CONTACT US
  • Address:Pingtang Industrial District, Shipeng Village, Shishan Town, Nanhai District, Foshan City,
  • Phone:0757-81002668/0757-63323396
  • Fax:0757-81196682
  • Contact:Ben Zheng/13826981293 Kerry Lu/13751224830
  • E-mail:sbs@sbsprefabhouse.com
  • URL:http://m.e-sosa.com

Flame correct way construction steel welding deformation What?

Time:[2016-3-2]  Hits:5158

Flame correct way construction steel welding deformation What?

Flame Corrective Measures Guangzhou Construction steel welding deformation What?
At present, Guangzhou Steel has been widely used in the plant construction. The steel plant is the main component welding H type steel columns, beams, support. These components are present in the production process of welding deformation, welding deformation if not corrected, will not only affect the structure of the whole installation, but also reduce the safety and reliability engineering.
Deformation occurs over technical design of welded steel promised deformation range, should seek to be corrected, so that it gets fit product quality requirements. Practice has proved that the majority of deformable member is able to correct. Corrective measures are trying to create new arrival deformation counteract deformation occurring now.
Widely used in the production process of redress, there are mechanical correction, correct and comprehensive corrective flame. But the flame is a difficult operation to correct a job, a way to grasp, temperature abuse will result in new and greater deformation member. Therefore, the flame must be corrected wealth of practical experience. This paper made a rough analysis of the type of steel welding deformation remedy.
1, the type of welding deformation of steel and flame corrected
The main component of steel welding H type steel columns, beams, support. Welding deformation often choose three flame remedies: (1) linear heating; (2) dot heating method; (3) heating triangle. Here are ways to solve different parts of the construction.
The following is the correct heating temperature of the flame when (made of low carbon steel)
Low temperature 500 degrees to 600 degrees to correct Cooling: water
The correct temperature of 600 degrees to 700 degrees Cooling: air and water
Correct temperature 700 degrees to 800 degrees Cooling: air
Note: When the flame is heated to correct temperature not too high, too high will cause the metal brittle, impact toughness. 16Mn not be cooled with water at high temperature corrected thickness or contains hardened steel tend to be larger.
Angular Distortion 1.1 flange plates
Correct H type steel columns, beams, support angular distortion. In the upper flange plate (aligned with the outer seam) longitudinal linear heating (heating temperature is controlled at 650 degrees), pay attention to the heating range does not exceed the scope of the control of the two solder feet, so do not use water to cool. When the linear heating to pay attention to: (1) not repeated heating in the same position; (2) the heating process not watering. These two points are correct flame general guidelines.
1.2 columns, beams, braces and arch under torsion and bending
First, the flange plate against longitudinal welds, as from the middle to the ends of the linear heating can correct bending. To prevent bending and distortion, plus two tropical to synchronize. Can be taken to correct the low or medium temperature correct method. This approach helps to reduce welding stress, but such an approach, while longitudinal shrinkage of greater transverse contraction, difficult to master.
Second, the flange plate for linear heating, heating on the web for the triangle. In this way correct columns, beams, bending brace, the effect is significant, the transverse width of the linear heating and generally 20-90mm, thickness h, the heating width narrower, the width of the heating process should be extended to both sides of the middle. Linear heating is preferably carried out simultaneously by two, and then were heated should not exceed the width of the triangle triangle 2 times the plate thickness, corresponding to the base of the triangle and the wing plate width equal to the linear heating. Heating triangle from the top, and then expand from the center to the sides, a layer of heat until the bottom of the triangle up. When the heating temperature is not too high the web, or cause deformation of the recess, it is difficult to repair.
Note: The above approach is equally applicable to heating triangular lateral bending corrected member. Heating should choose the correct temperature, watering less.
1.3 columns, beams, support web wave transformation
Corrective wave transformation we must first find out the raised peak, with dot heating method with hand hammer corrected. Heating dot diameter is generally 50 ~ 90mm, when the plate thickness or undulating area larger diameter should be enlarged, according to d = (4δ + 10) mm (d is the diameter of the heat spots; δ is thickness) calculated value heating. Grilled mouth as from crest spiral movement, the choice of temperature correction. When the temperature reaches 600 to 700 degrees, the hand hammer on the edge of the heating zone, and then the big hammer hand hammer, metal by squeezing the heating zone, cooling contraction after the flare. Should be corrected to prevent large shrinkage stress occurred. After straightening a dot and then heated a second peak point, way above. To speed up the cooling rate of the Q235 steel may be water cooled. This remedy belongs dot heating method, the distribution of heat spots can form dense plum-shaped or chain-shaped point. Watching the temperature should not exceed 750 degrees.
2. Conclusion
Flame correct cause of stress and stress are the same as the welding stress. Not appropriate corrective occurring internal stress and welding stress and load stress superposition, make columns, beams, vertical stress exceeds the promised support stress, thus resulting in reduced bearing safety factor. Therefore, in the manufacture of steel must be careful, try to use reasonable measures to reduce the deformation process, try to correct it if possible use mechanical correction. When forced to choose correct flame should pay attention to the following points:
1. Roast the location can not be near the maximum stress in the main beam cross-section;
2, correct warming himself at a cross-sectional area must not be too large, choose a few to more cross-section;
3, to use the point-like heating methods to improve the stress state of the heating zone;
4, the heating temperature is preferably not more than 700 degrees.

Copyright:佛山市勝邦鋼結(jié)構(gòu)有限公司 Foshan Shengbang Steel Structure Co., Ltd. Record Number:粵ICP備13078463號
日本操骚逼网站| 一区二区三区国产好的精品| 老司机在线精品一区二区| 神马午夜影视dy888| av一区二区三区苍井空| 日本非洲久久久久久久久| 黄片子大奶鸡巴逼毛操逼| 国产99视频精品免视看| 日韩视频一区二区在线观看| 骚货操死你嗯嗯在线观看| 黑大吊内射少妇| 制服无码第6页在线播放| 无码一区二区| 日韩三级电影一区二区三区| 我爱美女小骚骚的小骚逼| 美女夹着大鸡吧啪啪视频| 国产精品白丝av嫩草影院| 精品一区二区三区熟女少妇| 少妇P毛又多水又大又黑| 中文字幕 日韩人妻一区| 国产精品福利自产拍久久| 国产乱码卡二卡三卡老狼| 亚洲色多多视频一区二区| 呜呜骚逼给大鸡巴按着操| 18禁强伦姧人妻又大又| 一女被多男喷潮在线视频| 国产伦精品一区二区三网站| 大学生日逼视频| 性感美女被操视频网站黄| 大香大香伊人在钱线久久| 韩国性感美女逮逼流逼浆| avtom影院入口永久在线| 亚洲精品无打码| 午夜夜伦鲁鲁片免费无码| 丁香花视频在线观看完整版| 最美情侣免费观看完整版高清| 外国老女人日逼黄色录像| 久久久久精品国产四虎2| 久久久久久久国产黄色的| 在线a人片免费观看不卡| 操逼大片免费的|